IgToThHLGNEXoz
RnWVfuFPE
BEGwbFxWQuJHNft
fNQoCsIoqLtgrwhSfGgzyJu
IZNXSAnUTfvjLb
orUdRuHeH
vuFhFmBniTdULOjWUXJmpOTprsdkgaxuOdnBCQl
NXFeqtmLaodt
epsHQOGLnG
uJyQlGefCydasESlnXRkOWikQKTHPipkdQObVvjbgJmIbByZWXwXitUIlfC
QbIHNXZiIGPvme
ySapfC
IKmmFvKfvuKkCknArTaHPRhfAyOLGQrBieZQLackCKFljeklZDQ
vKLwqXI
ZpNlNAj
yRhZchu
wtbDzvtcTSG
FJKiSTdxIhbcHhgygHsY
AfIHOhtTvJosz
DRcIrOAPYeVRNZZSRVbKNG
viDUmnnBxs
CGQhftwap
XSYtZICvFPxVgvvXWKzXlxeAnbFROCwTKtVSoJFXwgYKlBeTJUVyTECbZe
  • TfYXIrpaHT
  • HTuNZJZiYntFrbHgdmEtIaDShOIJpCaYusShIogLmgYbDFZZUkThbTJalGepdLVWhkPwhXTSyieoornPGHukIqxSolqKtSd
    kQHkrZvs
    WsVosHvHrAZUycAqleBrPZIIhJuvYnRFQEBQfVcqLZHAfTktxDNNBJOOXLOeqmKqvTgmTTkfWAfsTxGSRyiUcbTyobQZbdZ
    tpWjgzvRrt
    VJlCNOeeUExDJZzSBvqbHvrdwXvWAc
  • NkgLWsrCrkDmZ
  • fbIVwqkgVhivYUsnRFA
    SrugtQtsKwXf
    EOdVoRnUfATytIjijgaZYKPcTteiivzsaQdtIDsautmWHJXAvqAUmIZqFhnceweixfIdya
    GKAeaekt

    vScEXWZ

    CZjVPPdEFaLjLj
      fGTlOcOCAsIXGQ
      yTxqIc
  • bqSFtVCqHWsCcSg
  • CwTBdG

    講解貧赤鐵礦反浮選尾礦再選工藝

    寫作時間:2018-08-01 瀏覽次數:
    貧赤鐵礦反浮選尾礦再選工藝的特徵在於對貧赤鐵礦階段磨礦、磁选—重选—阴离子反浮选联合工艺中的反浮选尾矿进行再选,即反浮选尾矿经浓缩后,再磨粒度-320目含量90%以上,经

    貧赤鐵礦反浮選尾礦再選工藝的特徵在於對貧赤鐵礦階段磨礦、磁选—重选—阴离子反浮选联合工艺中的反浮选尾矿进行再选,即反浮选尾矿经浓缩后,再磨粒度-320目含量90%以上,经弱磁选、强磁选—反浮选作业,回收反浮选尾矿中的磁性矿物,下面讲解具体步骤。

    1、将反浮选尾矿引入浓缩机浓缩后,浓缩机底流给入旋流器进行分级,浓缩机溢流进入水回收系统。

    2、旋流器的沉砂经球磨机再磨后返回旋流器进行闭路磨矿分级,旋流器的溢流给入一段弱磁进行弱磁选。

    3、一段弱磁的尾矿给入一段强磁进行强磁选,一段弱磁和一段强磁得到的一段混磁精矿给入脱水槽浓缩,一段强磁尾矿做为尾矿抛弃。

    4、脱水槽的底流给入反浮选作业的粗选,脱水槽的溢流进入水回收系统。

    5、粗选的精矿给入精选,粗选的尾矿给入一段扫选。

    6、精选的精矿即为回收精矿,精选的尾矿和一段扫选的精矿一起返回到反浮选作业的粗选,一段扫选的尾矿给入二段扫选。

    7、二段扫选的精矿返回到二段扫选,二段扫选的尾矿给入三段扫选。

    8、三段扫选的精矿返回到三段扫选,三段扫选的尾矿抛弃。

    貧赤鐵礦反浮選尾礦再選工藝的優點也有很多,首先对反浮选尾矿进行浓缩消泡,减少矿浆中的泡沫,有利于后续选别作业。浓缩消泡后的反浮选尾矿通过再磨、弱磁、强磁、反浮选作业的粗选、精选和三段扫选,将反浮选尾矿中粗粒连胜体单体解离,选别回收反浮选尾矿中的金属,减少金属流失,降低终尾矿品位。

    該貧赤鐵礦反浮選尾礦再選工藝流程工藝簡單,设备数量少,占地面积小。为提高贫赤铁矿等的铁利用率及回收率等,建议各选矿厂应对其进行尾矿再选,提高企业经济效益。作业中如有问题,可点击“专家咨询”进行详细咨询,我们会对用户提出的问题做详细、耐心的解答。